Quick answer: Case Screen-Print Adhesion clears on three checks: a 1 mm cross-hatch at 4B or better, 50 alcohol rubs under 500 g, and register inside 0.2 mm.

Table of contents

  • Five checks behind one verdict
  • Sampling: which wall, how many parts
  • Cross-hatch: spacing, cut count, peel angle
  • Alcohol rub: strength, load, stroke count
  • Grading and records: where the red line sits
  • FAQ

1. Five checks behind one verdict

Case Screen-Print Adhesion is settled by five steps in a fixed order: sample, lattice, rub, grade, record. Skip one and the later numbers mean nothing, because a sample taken at a rounded corner cannot be cut cleanly and the lattice reads low for reasons unrelated to ink.

A moulded case side carries a 1–2° draft, perimeter ribs and a parting line; the print sits on the flat band between the ribs, rarely flat to better than 0.05 mm. A blade crossing a swell cuts through in one square and stops short in the next.

StepActionCriterion
SampleFive cases at even spacingAll five present
Lattice1 mm spacing, 100 squares4B or better
Rub95% ethanol, 500 g, 50 strokesRe-test not below 4B
GradeTwo inspectors read apartBoth agree
RecordSeven columns into the batch sheetThree batches traceable

Five instruments cover Case Screen-Print Adhesion: a lattice cutter, 25 mm tape, a 500 g weight, a 10x loupe and a feeler gauge.

2. Sampling: which wall, how many parts

Five cases come off the finished pallet at even intervals, and nobody picks the best-looking one. The sample face carries the densest artwork, usually the lid front. Stay clear of a 3 mm corner radius, 5 mm either side of the parting line and 20 mm opposite the gate, where ink runs thin or thick.

Case Screen-Print Adhesion sample batch of grey and black cases stacked at the line end, pallet wrapped, assembly stations behind
Case Screen-Print Adhesion sample batch of grey and black cases stacked at the line end, pallet wrapped, assembly stations behind

Cure time sits inside the Case Screen-Print Adhesion sampling window. UV ink is tested 24 h after printing, solvent ink at 72 h; pulling tape earlier grades a film that has not finished cross-linking. When shop humidity reaches 80%, stretch that to 36 h so solvent leaves first.

Send a whole case or cut a 30 mm coupon from a reject. A whole case also lets the inspector read register; a coupon is quicker, but its sawn edge disturbs the tape.

3. Cross-hatch: spacing, cut count, peel angle

Spacing follows dry film thickness. Under 50 µm it is 1 mm, from 50 to 125 µm it is 2 mm, and above 125 µm the test switches to the X-cut. Screen ink on a case lands between 8 and 30 µm, so every job sits in the first band: 1 mm spacing, 11 cuts one way and 11 the other, leaving 100 squares.

Depth is the hidden variable. The blade passes through the ink and just touches plastic; gouging 0.05 mm into the substrate starts a crack that lifts neighbouring squares, while a dull blade skates and leaves uncut squares attached.

Brush the debris off with five diagonal passes each way, apply 25 mm tape, roll it down three times, wait 30–60 s, then pull at 90° within 0.5 s, once per site. A second pull on the same lattice says nothing about Case Screen-Print Adhesion.

ClassArea removedDisposition
5BSmooth cuts, no squares offRelease
4BFlakes at intersections, under 5%Release on visible faces
3BFlaking along edges, 5%–15%Rework or re-judge
2BRibbons of coating, 15%–35%Scrap
1B and 0BOver 35%, whole squares goneScrap, audit pretreatment

4B is the Case Screen-Print Adhesion release line and 5B is kept for faces carrying a customer mark. Before scrapping a 3B lot, check pretreatment: polypropylene and polyethylene sit at 29–31 dyn/cm and hold ink only after flame or plasma treatment, while ABS and PC print as moulded, so 3B there points at release agent.

4. Alcohol rub: strength, load, stroke count

Use 95% ethanol, wrap two layers of cotton around a 500 g weight, run a 60 mm stroke at one cycle per second for 50 strokes, and halve that to 20 on corners. Rub across the lettering, not along it; a stroke that follows a printed line carries the whole line away.

Case Screen-Print Adhesion screens standing in layers on blue racks, green-painted wooden frames numbered, yellow floor lines in the aisle
Case Screen-Print Adhesion screens standing in layers on blue racks, green-painted wooden frames numbered, yellow floor lines in the aisle

Let the panel stand 10 min so the ethanol flashes off, then cut a fresh lattice at the same site. This is a re-test, not a second opinion: the class may drop one step at most, and anything under 4B fails. Lots that skip the rub fail the day a customer wipes the case with a swab.

Hold the room at 45%–55% RH. Below 40% static pulls dust onto the print and the removed area reads high; above 65% the film re-tacks and the re-test reads low. Both errors misstate Case Screen-Print Adhesion.

5. Grading and records: where the red line sits

Three numbers form the red line: 4B on the lattice, 0.2 mm on register, 15 N/cm on screen tension. Break one and the lot stays out of the finished-goods store.

Register is measured on a pinned fixture. Single-colour artwork holds ±0.1 mm against a moulded datum, two-colour work is allowed ±0.2 mm, and multicolour work keeps a 0.2–0.3 mm trap so the second colour lands on the first without a white gap. Past 0.2 mm the doubling shows at 30 cm; the cause is tension.

Keep working screens between 18 and 30 N/cm and retire them below 15 N/cm. A slack mesh shifts under squeegee pressure, so the first 200 units register and the next 200 drift. Set off-contact at 1.5–3 mm: widen it and squeegee pressure rises, the film thickens, and a thicker film passes 4B more easily.

Test the first piece of every batch, then add five cases per 2000 units. Three consecutive 5B batches allow five per 5000; one 3B sends frequency back to five per 500.

The Case Screen-Print Adhesion sheet carries seven columns: batch, screen number, ink lot, cut spacing, tape grade, lattice class, re-test class. Seven columns rebuild the Case Screen-Print Adhesion history of a case three months on; six leave the rework call to memory.

Conclusion

Case Screen-Print Adhesion is a chain, not a grade. Lock spacing at 1 mm, the rub at 95% and 500 g, register at 0.2 mm, and classes become comparable. Fill all seven columns and the next drift surfaces before a customer finds it.

This article covers only the specification and design meaning of the container (case) side, and does not address any handling, loading or use of the contents.